SampleHDPE-WT-004
Plastic TypeHigh-density Polyethylene (HDPE)
Molecular Formula(C2H4)n
ColorWhite
Common useShower gel bottle
Degradation details Exposure to indoor conditions – it was only used as a shower gel bottle for 3 months and then it was measured After indoor degradation, the sample was degraded in environmental conditions (for 3 months) such as wind, rain, snow, temperature variations and sun radiation.
Time of degradation3 months of indoor degradation + 3 months of environmental degradation
Sample description The sample is rigid, clean with no visible signs of degradation after indoor degradation, but after environmental degradation, the sample was covered with dirt and water.
Bellow you can find the Raman spectrum of the sample before and after the environmental degradation.
Microscopic image(s)
Macroscopic image(s)
Spectral Data typeRaman
Raman spectrum acquisition parameters
(for both spectra)
Laser wavelength: 785 nm
Laser Power: 300 mW (100% of the laser power)
Exposure time: 1 s
Objective magnification: 20X (NA 0.35)
Spectrum range: 765-1600 cm-1